Materials | High chromium cast steels and cast irons

Due to their relatively suitable wear resistance and toughness, high chromium cast steels are used widely in grinding processes. Considering the application, this group of martensitic steels has filled the gap between manganese steels and high chromium cast irons with its suitable impact and high abrasion resistance.

Alternatively, high chromium cast irons are universally applicable to conditions where excessive wear and moderate impact are present.

This group of white cast irons will provide superior wear resistance because of their martensitic matrix, which is enriched with carbides. For conditions that marginal impact and superb abrasion resistance is essential, nickel chromium (Nihar4) white cast iron will be appropriate.


Symbol

 

Basic Chemical  Composition

%C

%Si

%Mn

%Cr

%Mo

%Ni

TWRC10

(Max)

0.4

(Max)

0.7

(Max)

1.1

5.0

7.0

-

-

TWRC11

(Max)

0.4

(Max)

0.7

(Max)

1.1

6.0

8.0

      -

-

TWRC12

(Max)

0.3

(Max)

0.7

(Max)

0.9

10.0

13.0

-

 -

TWRCOA

1.1

1.4

(Max)

0.8

(Max)

0.8

11.00

14.00

-

-

TWRCO

1.4

1.6

(Max)

0.8

(Max)

0.8

11.0

14.0

-

-

TWRC2

2.3

2.9

(Max)

0.8

(Max)

1.5

18.0

20.0

0.0

2.0

0.0

2.0

TWRC5

 

2.3

2.9

(Max)

1.0

(Max)

1.5

25.0

28.0

0.0

2.0

0.0

2.0

TWRC6

 

3.0

3.5

(Max)

1.0

(Max)

1.5

23.5

28.5

0.0

2.0

0.0

2.0

TWRN4

 

2.5

3.5

(Max)

2.2

(Max)

0.8

7.0

9.0

-

4.5

6.5


 
Copyright Tabrestan Steel Foundry, .2009 ©